Part A |
|
|
hatting agent |
2.0 |
|
ethanol |
2.5 |
|
ethyl glycol |
3.0 |
|
Part В |
|
|
water |
6.0 |
|
melamine resin |
21.0 |
|
pine oil |
0.4 |
|
tri-butyl phosphate |
0.5 |
|
slip agent |
0.5 |
|
de-foamer |
0.1 |
|
Slowly stir A into В |
|
|
Part C |
|
|
hydroxy acrylate emulsion |
50.0 |
|
silicone oil (50% in water) |
0.5 |
|
dimethylethanolamine (to pH = 7.5) |
0.2 |
|
water |
11.8 |
|
sodium hexametaphosphate (10% in water) |
1.5 |
|
Total |
100.0 |
|
FORMULATION 7-8 |
Add A/В mixture to C, filter and add immediately prior to use para-toluene sulphonic acid solution to pH = 1.5.
![]() |
![]() |